By Ted Moores

The WEST SYSTEM User Manual
& Product Guide describes the basics of fiberglass cloth application and
coating for clear finishing over wood. This article is the ultimate guide to
applying fiberglass over a woodstrip hull to achieve a perfect finish. Ted Moore
is a master of the perfect finish, author of CanoeCraft and KayakCraft and
co-owner of Bear Mountain Boats.
The secret to a clear coating is to control the film thickness of each layer of
epoxy as it is applied. Building up the epoxy/glass over the wood may be
compared to making a mirror. The prepared surface of the wood is the back
reflective coating and the epoxy/glass is the glass or lens. In order to reflect
the clearest image of the planking, the lens must be clean, smooth and of a
consistent thickness. It is impossible to think of applying the epoxy resin in a
haphazard manner and expecting to sand it back to a consistent film thickness.
Also, when the epoxy builds up thick all at once, air is trapped inside and will
appear as a white blemish or streak. If it is in the first coat, there is a good
chance it will be in or below the surface of the cloth. Sanding will not remove
these blemishes without cutting into the glass fiber, thus weakening the
structure
Building the layers up evenly will involve a different technique for each layer. Each
layer accomplishes a specific function and is controlled by specific
limitations.
On the outside of the hull where durability and visibility are prime
considerations, three layers of epoxy resin and one layer of glass fabric are
used. The glass fabric is always laid up in the first coat of epoxy, the second
fills the weave and levels the surface, and the third buries the fabric, giving
enough depth of resin to sand smooth without hitting the cloth.
On the inside, consider omitting the third coat of epoxy. This surface will be less
slippery yet look good. Also, this eliminates about 90% of the sanding of epoxy
on the inside, a step that could be expected to take about one day to complete.
The trick here is to be extremely careful squeegeeing the first and second
coats. The texture of the weave must be consistent in order to look good. Think
about this when you are squeegeeing the outside; this is a good place to
practice getting an even texture.
Tools and materials
While technique and attention to detail are important for a good finish, it is also
essential have the proper materials and have them on hand at the right time.
Buying fiberglass cloth
It is important that the finish on the fiberglass cloth be compatible with the
resin that you are using. After the glass fibers have been woven into cloth, it
is fired to remove all the residual wax and oil and is then finished with a
<%-2>coupling agent. The coupling agent is the interface between the glass
fibers and the resin. Sticking well to both the glass and the resin, it keeps
the bond from deteriorating. There are many different finishes available, but
few are compatible with epoxy for our purpose. To be sure, buy your cloth from
your epoxy dealer and ask if the finish is compatible with the epoxy.
When you buy cloth, insist that it be carefully rolled. If it is folded, the creases
will not come out. On the outside, there is a chance to sand them flat with the
possibility of hitting the glass and having to patch it. On the inside if only
two coats of resin are used, the wrinkle will remain visible.
Brushes
Look for a cheap natural bristle brush 2½" or 3" wide with short bristles
that are not too thick. A good varnish brush would not be a good choice as it
holds a great deal of material. This is not only wasteful, but it is also hard
to clean out. Old epoxy collects up inside and hardens before the project is
complete. Because of its greater viscosity, epoxy resin should not be expected
to flow out of the brush as freely as paint or varnish.
Beware of ultra cheap “Chip” brushes with blonde bristles. They shed like a dog
with the mange and the bristles are almost impossible to see on light colored
cedar. All brushes are going to shed some when they are new, but a dark bristle
will be easier to see. Shake out as many bristles as you can before using the
brush for the first time.
Take care of the brush. It gets better the more it is used. When you are finished
using the brush or you feel it beginning to get stiff, scrape the excess resin
out of the brush into a grunge can and then rinse it in lacquer thinner. Store
the brush in clean lacquer thinner between coats and when finished coating, wash
it with soap and water or a water soluble brush cleaner. Acetone will work as
well as lacquer thinner, but I find the smell offensive and it seems to
evaporate faster.
Rollers
Rollers sound like a good idea and almost work. However, when used for applying the
epoxy to the dry cloth, there are several problems. It is tricky getting enough
resin on to wet out the surface of the wood and the fabric. As the resin is
squeezed out of the roller, air comes with it and gets trapped in the weave of
the cloth. Also, the cloth has a tendency to stick to the roller and roll up as
the roller passes over it.
For applying the second coat of epoxy the roller is useless, as the weave is very
coarse and will cause the resin to foam up.
On the third coat, the roller will work. After rolling the epoxy out evenly over a
2' or 3' section, work the surface gently with the tip of a dry brush to break
the bubbles. If you do use the roller for the third coat, a fourth coat would be
worth considering as the roller does not build up the coating thickness as fast
as the brush will.
Resin/hardener dispensing pumps
It is worth having a set of dispensing pumps that will give the correct ratio of
resin and hardener with one stroke of each pump. WEST SYSTEM® mini
pumps come with a volume/ratio tester. Use it. If there is a problem later, the
question of the pumps’ reliability will be eliminated.
Squeegee
Treat this piece of plastic as a precision tool. It is the key to a finish that looks
like 12 coats of varnish. Check the edge for nicks and repair and soften the
edge with 220 sandpaper.
Rags
Use white, lint free cotton. Old white cotton bed sheets are ideal. Avoid colored
fabrics as the dye could be dissolved by the lacquer thinner and transfer to the
surface.
Grunge can
One of the problems encountered using the squeegee is what to do with the waste
resin (grunge) after it is picked up with the squeegee. If the waste is not
removed from the squeegee after each pass, it is transferred to the beginning of
the next pass. This leaves a line of waste resin where it should be clean. The
can of choice is the rigid cardboard frozen juice can (photo
below).
Cut a slit ¾" down from the top edge and draw the squeegee through the slit.
Both sides of the squeegee will be perfectly clean and the grunge will have run
into the can. The length of the slit is important: if it is too deep, the sides
of the can will spread and you won't get a clean scraping action.
The next problem is what to do with the grunge that is in the grunge can. As the
volume of old resin builds up in the can, it will begin to heat up quite
rapidly. At some point it will boil out over the top and run down the side. Not
only could this be very painful, but the fumes are toxic.
When you begin to feel the heat building up through the side of the can, dispose of
the waste resin in a large disposal container with 2" or 3" of water
in the bottom. The water will dissipate the heat and keep it from boiling. A
large 2 liter disposable soft drink container with the top cut off will work
well and you can watch the resin harden into some interesting shapes in the
water.
Working with epoxy and fiberglass
The optimum working temperature is about 70° F. If you are comfortable in a
"T" shirt, it should be about right. At about 80° F, the working time
will be reduced dramatically so watch the time between applying the resin and
when you squeegee off the excess.
Pick a time of day to begin the lay up that will give you the most comfortable
working temperature. The second and third coat are affected less by the
temperature and will be controllable in less than ideal conditions.
Assemble all materials and supplies and set aside a block of time when you will not have
to deal with distractions. This is a one shot deal and deserves your undivided
attention.
Clean the surface of the hull with a rag dampened with lacquer thinner to pick up the
dust. This is not a washing step. Use only enough thinner to dampen the rag
enough to hold the dust onto the cloth.
Roll the cloth out over the hull leaving about 6" extra at each end. With a
person at each end holding the cloth in the middle, pull the cloth back and
forth in a seesaw motion to center the cloth on the hull. While holding the
cloth at the middle with one hand, use the other hand to work down to the edge,
tugging against your partner ever 4' or 5'. This exercise will shape the cloth
perfectly around the hull. You should be able to manipulate the entire piece of
cloth from the end.
Use this technique if wrinkles develop in the cloth during the lay up. Trying to
brush them out with your hand could put a permanent crease in the cloth.
Mixing epoxy
This is a good part of the project to have some help on. Break the duties down to
mixer and applicator. They are both critical positions although if it is your
boat, you may want to be the one in direct control of the visual aspects by
applying and squeegeeing the resin. Don't let anybody distract the mixer!
Mixing
requires great responsibility and concentration. There is no graceful solution
to leaving one shot of hardener out of a batch that is being applied to the
cloth. On the second coat, the resin could be washed off, but when it is in the
cloth, more drastic solutions must be considered.
Get into the habit of dispensing the resin first, followed by the hardener. Count to
yourself or out loud if it helps: one (resin) one (hardener), two (resin) two
(hardener), etc. Keeping to a system will reduce the odds of getting lost. If
for some reason you have doubts about the accuracy of the ratio, discard the mix
rather than take a chance on spoiling the lay up.
When choosing the number of shots per batch, there are several things to consider.
Once the resin and hardener are combined, a chemical reaction begins that
produces heat and this heat produces more heat. The larger the batch, the faster
the heat will be generated. As the heat builds, the epoxy loses viscosity and
begins to thicken. This thicker resin will not soak into the surface of the wood
or the glass fibers as far as the thinner, fresh resin will. You will see this
as a lighter shade on the planking and the glass fabric could be visible. If you
feel the resin beginning to heat up, discard it.
Batch size/mixing time/working time
1st coat, dry fabric—4 shots or ½ cup
2nd coat, filling the weave—2 shots
3rd coat, brush or roller—3 to 4 shots
Always use fresh resin. Tell the mixer just before you run out so that there will be a
fresh batch of resin ready at the same time that you run out.
Stir the resin/hardener mixture for at least 45 seconds, more if the resin is cool
and stiff. Scrape the sides and bottom corners often and reverse the stirring
direction from time to time.
WEST SYSTEM® 105/207 has a pot life of about 15 minutes at 70°F, less as
the temperature goes up, more as it goes down.
If during the lay up you notice that the brush is getting stiff up around the
ferrule, take the time to scrape out the old resin and rinse the brush in
thinner.
It is a good idea to scrape the excess resin out of the brush every 3 or 4 batches
or when you see a lot of foamy resin in the brush. This will help to keep all
the resin in the brush closer to the same age.
Applying the first coat of epoxy
Applying the epoxy resin to the hull surface will require a different brush technique for
each coat.
The function of the brush on this coat is to transfer the resin from the can and to
spread it gently over the dry cloth. There should be no attempt to work the
resin into the cloth as this will introduce air bubbles into the resin that may
or may not come out when it is squeegeed. Load the brush and spread with
controlled but bold strokes (photo below).
As you work aggressively ahead, keep an eye on the area that has just been
covered. Watch for places where the cloth looks dry or starved and add fresh
resin rather than pulling a run of questionable age over to it. Don't mess with
the runs a whole lot as they will be removed later with the squeegee.
This is one place where working aggressively with disregard for neatness is the most
appropriate thing to do. The fresher you can keep the resin at the edge, the
more consistent the color will be.
When you dip the brush, there will be resin on both sides of brush. Turn the brush
over to transfer the resin from both sides of the brush to the surface.
As the resin soaks in, notice how the cloth has become visible first around cracks
and staple holes. The cloth works as a wick, effectively feeding resin into the
voids.
The surface of each plank will absorb the epoxy resin at different rates. It is
important to supply enough resin to give each plank as much as it wants. Watch
for dark heart wood planks as they seem to absorb more than light colored
planks.
Where to begin
When deciding where to begin applying the resin, the main consideration is keeping
the edge of the resin fresh as you precede down the hull wetting out the cloth
(photo below). This will depend of the size of the hull and the
number of people involved.
If you are working with just one person applying the resin, begin at the keel line
about 3' back from the end. Work down to the sheer and out to the end. This will
tighten up the cloth and move the excess cloth out to the end of the hull.
Repeat on the opposite side of the hull. Then move back to the side you began on for
the third section. Change sides with each section of about 2' to 3' as you work
down the hull.
When the first section has been wet out, use this section as an anchor, working away
from it to avoid bunching up the cloth.
By the time you get to about the halfway point, the area first wet out should be
ready for squeegeeing. It is important to squeegee only the first area, as the
section beside it will be 5 to 7 minutes behind.
You will alternate between wetting out one section and squeegeeing one section. If
the mixer has a good idea of how you are applying the resin, he or she could
fill in applying the resin until you catch up.
Using the squeegee
This might be the trickiest step of the whole process and it governs what your boat will look like. It is
very difficult to reverse and you need to be able to do it right the first time.
While it is not a difficult step, you need to give it your full attention while
you are doing it.
The purpose of the squeegee is to even out the film thickness by scraping off the
excess resin (photo above). The
planking has now accepted all the resin it wants; the cloth is saturated but
floating in places. Squeegeeing will leave the cloth evenly saturated and lying
flat on the hull.
Holding the squeegee
As most plastic squeegees have a slight curve along the edge, hold it so that the
corners turn up. Turned over, the corners will dig in and scrape too much resin
out of the cloth. Hold it so that your thumb is on the bottom side and your
fingers are spread out to control the pressure along the edge.
The angle that the squeegee is presented to the hull is most critical. The angle
should be quite flat with your thumb almost dragging on the hull. A steeper
angle will put too much direct pressure on the cloth and too much resin will be
scraped out. Be conscious of keeping this low angle as you go around the turn of
the bilge. There is a tendency to allow the angle to get steeper as you come
around the turn of the bilge.
Applying the right pressure
If too much pressure is applied, too much of the resin will be squeezed out of the
cloth. This is undesirable as after the resin sets up, the fibers of the cloth
will be coated and sealed but not filled. The second coat will not be able to
penetrate the fibers any further and the glass fibers will remain visible. This
will be most noticeable in bright sun light on dark wood.
If you don't press hard enough, the surface will remain shiny and the cloth will be
floating. In practice, it is a good idea to work a section down in stages rather
than trying to get it all in one pass.
Working the squeegee
Begin at the centerline (keel line) of the hull and draw the squeegee down to the
sheer with overlapping strokes. The speed should be slow enough to allow the
resin to roll up in front of the squeegee.
The amount the successive passes overlap will depend on how much resin is being
removed. If there is a lot of resin, pick up only as much as you can hold on the
squeegee and transfer to the grunge can. As you get closer to the desired film
thickness, use the full width of the squeegee.
Work gently over the section until the vertical shiny tracks are removed. In
practice, you won't get all of them, but try to get as even a texture as
possible without wasting too much time. Keep in mind that this is practice for
getting an even texture on the inside where it will be more visible.
As you work these last tracks out, be very conscious of not taking too much and
starving the cloth. If too much resin is removed, the cloth will have a subtle
white glitter rather than a saturated dull shine. Should this happen, add fresh
resin rather than dragging old resin over to it.
Finishing the cloth at the stems
Wet the cloth out on both sides. Then trim it to about 1" past the end of the
stem. Check that the cloth is lying down flat to the hull along the edge. After
the resin has firmed up (about 3 hours), trim it off clean with a sharp knife
and soften the edges with 120 sandpaper.
Applying the second coat of epoxy
The purpose of the second coat is to fill the weave and level the surface of the
cloth (photo below). No attempt should be made at this point to build up
the resin thickness. The surface is too coarse to brush on without the resin
foaming up as well as the danger of air being trapped at the bottom of the
weave.
The minimum time between coats is about 3 hours or when you are able to trim the
cloth without the resin sticking to the knife. The three coats should go on as
close together as possible. Applying before the previous coat has cured will
result in a chemical bond as well as a mechanical bond.
If you can time it right (about 4 to 5 hours), a quick hand sanding with 120 grit
will take the tooth off and make the surface easier to work on. Since the depth
of the weave is being reduced, slightly less resin will be required to level the
weave.
If it has been more than about 8 hours since the last coat was applied, the surface
should definitely be sanded. This is important because the integrity of the bond
between the layers now depends on the layers being mechanically bonded together.
How to apply the second coat
On a horizontal surface or on the inside, it is possible to pour a small puddle of
resin on the surface and then spread it around with the squeegee. The technique
that works for me on the outside is to use the brush to transfer the resin from
the container to the hull. Since the brush is depositing more resin than is
necessary to fill the weave, only spread the resin about 1/3 of the way down
from the centerline. This should be just enough resin to fill the weave all the
way down to the sheer line.
The first time over, concentrate more on filling the weave than making it look good.
Work the resin aggressively enough to force the trapped air out of the craters
in the weave.
After roughly spreading each batch, go back over the section systematically, scraping
off and disposing of the excess resin.
Use a steeper angle and slightly more pressure on the squeegee this time to force
the air out and to level the surface.
The part that is most likely to get missed is the vertical surface along the sheer
line. Check for dull patches that would indicate an area that has been missed.
It is hard to see on the vertical surface so check from all angles.
Listen to the squeegee. As it passes over a dry patch, you will hear a harsher sound.
If there is a problem getting the vertical tracks out, try working in a fore and
aft direction. On the inside where you want to get rid of all the tracks, go
over the surface with a dry brush. This may be a reasonably aggressive motion in
a fore and aft direction.
Check that the ends of the stems have been coated evenly.
Applying the third coat of epoxy
The purpose of the third coat is to bury the glass cloth with enough epoxy resin
that the surface may be sanded smooth without hitting the cloth. Even though the
surface has been squeegeed and the cloth is buried, expect to see a slight
profile of the weave after the third coat (photos
below).
How to apply the third coat
This coat will be applied with a familiar painting motion. Since you are now working
on reasonably smooth substrata, a more aggressive motion may be used without
introducing air into the resin. If you do see bubbles forming excessively, be
less aggressive.
The idea is to apply as much resin as you can get on in an even film thickness
without it running. You will have to use your judgment to find this balance
between just right and too much. Too much will give the brush a mushy, skidding
feel while too little will have noticeably more resistance. Controlling the film
thickness by feel is often more reliable than doing it visually, especially if
the light is marginal. In practice, you will use a combination of both what you
can see and what you can feel.
Load the brush and apply to a section about 3' long or as long a section as you can
work comfortably. Spread with a long vigorous but controlled back and forth
motion to work the resin out into an even film thickness. Check for even film
thickness by brushing up and down, feeling for consistent resistance through the
brush.
After spreading the resin over the section being worked on, go back to where you
started and finish off with long, flowing fore and aft strokes. This motion
should be like an airplane landing and taking off gently to help the resin blend
in evenly with the adjoining sections.
When applying resin beside a completed section, work from the wet to the dry to keep
the resin from building up too thick along the overlap.
There is a limit to how long you can play with working the runs out. At some point,
the resin will begin to firm up and will pile up and not flow out. This is the
time to quit because from this point on, working it will only make it worse. A
premium resin system like WEST SYSTEM 105/207 has good self-leveling properties.
While this is desirable for getting rid of brush marks, it is also what causes
the resin to run. Don't take a few runs on this coat too personally as they
happen to all of us. Remove the runs after the resin has cured with a sharp
cabinet scraper. Trim the excess cloth after the third coat has hardened (photos below).
When the final coat has cured thoroughly, sand to prepare the surface for varnish,
beginning with 80-grit paper and finishing with 120-grit. Apply four coats of
premium spar varnish for UV protection.