Auto bodywork: A quicker fix with G/5 adhesive
By Brian Knight

A small area in the rear quarter panel of my wife's car was perforated from rust. I cleaned the area
using a Nyalox™ abrasive impregnated nylon bristle brush (Photo 1) to remove as much corrosion as
possible-including the back of the repair area.
To quickly make a backer for the hole, I used G/5 Five-Minute Adhesive. I impregnated a small piece of
6 oz fiberglass cloth with G/5 and spread it flat on a piece of Melamine board. After about five minutes,
the cured backer peeled from the surface of the Melamine. I trimmed it slightly larger than the hole in
the fender and inserted a screw in middle of the backer so I could pull it into place when I installed
it. I then coated the inside edges of the hole with a mixture of WEST SYSTEM® 105/205 epoxy thickened
with 410 Microlight (Photo 2) and flexed the backer slightly to fit it through the hole. I pulled the
backer into the thickened mixture, which held it until the epoxy cured. With the backer in position,
I removed the screw and completed my repair. I roughened the surface with 80-grit sandpaper and
applied a layer of 105/205 thickened to a peanut butter consistency with 410 (Photo 3). I rough shaped
this layer after it cured and then applied a thinner coat of the same material. After this was cured
and perfectly faired, I coated the entire repair area with unthickened WEST SYSTEM epoxy and wet
sanded. Finally, I applied primer and spray paint using a Preval™ sprayer (Photo 4).
Sources: Nyalox™ abrasive impregnated nylon bristle brushes, Dico Products Corp., Utica, NY 13503
(purchased at The Home Depot™).
Epoxyworks 17 / Spring 2001
Copyright © 2002, Gougeon Brothers, Inc. All rights reserved.
This page is maintained by Gougeon Brothers, Inc. Last Modified on 10/28/02.
Reproduction in any form, in whole or in part, is expressly forbidden without the consent of the publisher. EPOXYWORKS, Gougeon Brothers, WEST SYSTEM, Episize, Scarffer and Microlight as used throughout this publication, are trademarks of Gougeon Brothers, Inc., Bay City, Michigan, USA.
|