Many of us at Gougeon Brothers experiment with WEST SYSTEM® products on personal projects at home as well as at work. We often push products and techniques beyond the limits recommended in our literature. Sometimes the experiment fails, sometimes we discover something very useful.

Installing ceramic tile
Grant Urband, head of our marketing department, developed an interesting approach for using G/5 Adhesive during an interior restoration project on his Victorian era home. He recently used G/5 to glue hundreds of 1" square ceramic tiles to a large surface and in the process, came up with a unique method for using the fast-curing adhesive.

Any time you must continually repeat a process, it is worth developing techniques that improve your efficiency. Grant knew that he would have to use small batches for this project because of G/5's short working time. After experimenting with several batches, he discovered that G/5 resin and hardener can be dispensed into small mixing cups ahead of time and will remain uncured until mixed.


He made a carrying pallet with sixteen holes, sized to hold 1-ounce mixing cups (pill cups purchased at a food service outlet). The pallet was covered with duct tape so glue drips could be peeled away (above).

He arranged all of his materials close at hand.

  • A pallet with pre-filled mixing cups
  • Mixing (popsicle) sticks (purchased at a crafts store)
  • 403 Microfiber Filler
  • Ceramic Tiles organized in order
  • Supply of disposable gloves

He simultaneously dispensed the resin and hardener into opposite sides of each cup. Although the resin and hardener lay against each other, no reaction occurred until the contents were stirred together (below).


Once Grant's project was underway, he was able to quickly mix new batches and work continuously without stopping to dispense resin and hardener.

Plastic repair with G/5 Adhesive
I occasionally use my tools on jobs for which they were not intended. I won't go into detail, but it was on one of those occasions that I significantly damaged my ratcheting "squeeze driver" screwdriver. The plastic that surrounded the thrust bearing had broken into several pieces. I didn't know if it could be repaired but I was going to give it a try.

I decided to use G/5 Adhesive for this repair, since it adheres quite well to a number of plastics. I planned to incorporate 4-oz fiberglass cloth to reinforce the area around the thrust bearing after gluing the pieces together.

These are the basic steps I used:

  1. Dry assemble the unit to verify all of the pieces are there (left photo).
  2. Prepare the repair for fiberglass and epoxy by sanding with 60-grit sandpaper.
  3. Oxidize the bonding surfaces with a brief pass of a flame from a propane torch.
  4. Glue the pieces together with G/5 Adhesive.
  5. Laminate layers of 4 oz fiberglass cloth with small multiple batches of G/5 to reinforce the damaged area (middle photo).

I guess you can say the repair was successful. It's been a year and a half and my "squeeze driver" works fine (right photo). I think it is stronger now than when it was new. It may even work on jobs for which it wasn't originally intended.

Epoxyworks 20 / Fall 2002

Copyright © 2002, Gougeon Brothers, Inc. All rights reserved.
This page is maintained by Gougeon Brothers, Inc. Last Modified on 10/28/02.
Reproduction in any form, in whole or in part, is expressly forbidden without the consent of the publisher. EPOXYWORKS, Gougeon Brothers, WEST SYSTEM, Episize, Scarffer and Microlight as used throughout this publication, are trademarks of Gougeon Brothers, Inc., Bay City, Michigan, USA.