Bonding fasteners in high-density urethane foam

By Bruce Niederer
Many of our readers who are familiar with WEST SYSTEM® Brand epoxy products for building and repair
already know the benefits of fastener bonding techniques. WEST SYSTEM epoxy has been used in other
industries for many years as well, and these folks apply knowledge and techniques developed in the
marine and aerospace industries in their work. A good example is the sign industry, a huge industry
in the U.S. with companies ranging from mom & pop garage operations to multimillion-dollar corporations.
The materials used to make signs are as varied as they are to make boats and planes: wood, metal,
plastics, composites and, the focus of this article, high-density urethane (HDU) foam. HDU is used
because it is lightweight, easily shaped, and cost effective. But one of the problems with foam signs,
particularly in outdoor applications, is how to attach them to a wall or frame so they stay put through
all types of bad weather. The fastener bonding technique developed and recommended by Gougeon Brothers,
Inc. for marine hardware using WEST SYSTEM products is perfectly suited to HDU foam sign building.
Fastener bonding technique
The basic idea behind the technique is to drill oversized holes in the foam, fill the holes with
thickened epoxy, and mount the fasteners in the epoxy. It really is just about that simple, but if
that's all there was to it, this would be a darn short article-so let me elaborate. We have learned
from our boatbuilding experience that if a load on a fastener is spread out over a larger surface area
than presented by the fastener itself, in any given substrate material, a larger load can be carried.
So how can this principle be applied to an HDU foam substrate and why should anyone bother? To answer
this question, I wanted to quantify and compare the strength of a fastener bonded with the fastener
bonding technique to one that wasn't. So I set out to devise a few simple experiments.
Identifying the engineering issues, that is, the type of loading the fasteners might experience, was
the first step. Visiting some websites, I quickly learned that HDU signs are hung from the back (single
or double post or from a wall), from the sides (usually double post), and from the top. This means the
fasteners could be loaded in tension, as from top mountings, or in a combination of peel/shear loading,
as from back, side or wall mounting. Each type of mounting would also need to withstand durational
loading, commonly referred to as creep loading, as well as cyclic and shock loading. These are all
typical loads fasteners experience in the marine and aerospace environments.
3 key elements of fastener bonding strategy
- Drilling an oversized hole about twice the diameter of the fastener.
- Encapsulating the threads of the fastener in WEST SYSTEM epoxy thickened with 404 High-Density
Filler.
- Using a mold release on the threads of the fastener.
There are slight differences in technique between bonding screws and bolts.
For screws, drill an enlarged hole about 2/3 the length of the threads that will be covered in the epoxy.
Then drill and center a shallow pilot hole in the bottom of the larger hole. Coat the threads with a mold
release (see the sidebar at the end of this article). Mix epoxy filled with 404 High-Density Filler to a
catsup consistency, and then pour into the hole, filling it about half way. Place some of the filled
mixture on the threads to avoid trapping air on the threads and then screw into the pilot hole. This
centers the screw in the center of the enlarged hole. Finally, either clean up the excess that squeezes
out or add a little more epoxy with a syringe. Allow the epoxy to cure.
For bolts or threaded rod, the procedure gets modified somewhat. After applying the mold release, place
two nuts on the rod-one at the bottom of the threads and one above. This time drill the oversized hole
the diameter of the outside points of the nuts. The reason for this is that when the rod and nut assembly
is inserted into the hole, it is automatically centered. Additionally, the threaded rod can be turned in
and out repeatedly without relying only on molded epoxy threads, which will begin to chip and crack after
several cycles in and out. Finally, the top nut is positioned so that its top is just proud of the surface
of the foam, so hardware can be tightened against the nut, not the foam or epoxy. Tightening against the
foam or epoxy pre-loads the materials before the loads the fastener is designed to carry are even applied.
The testing
To begin the testing, I mounted fasteners in 15 pcf (pound/cubic foot-see the side bar) HDU-a ¼" screw
without any epoxy into a properly sized pilot hole and 3/8" threaded rod with 2 nuts and epoxy as
described above. I used our PATTI instrument (Pneumatic Adhesive Tensile Testing Instrument) to pull each
fastener to quantify the force needed to remove it from the foam. This test is intended for ASTM Standard
D4541, which tests adhesive coatings. To be valid for this application, I calculated the bonding surface
described by the area of a cylinder. For the screw, I measured the outside diameter of the threads. The
results were dramatic. It took a force of 479 lb to extract the ¾" epoxy annulus and only 143 lb to
extract the ¼" screw. What this test is actually testing is the shear strength of the HDU foam itself.
The epoxy annulus being larger incorporated more surface area of the foam and so required more than 3
times the force to break a larger area of foam.
Next, I mounted a 3/16" eyebolt with 2 nuts in 18 pcf HDU foam as described above. After allowing it to
cure 24 hrs, I secured it to a vertical frame and hung weights from it (photo 1). This loaded the fastener
in a combination of shear and peel at 90°. This test also incorporates creep into the loading profile. I
started with 40 lb for 24 hrs, increased to 60 lb for another 24 hrs, and then to 80 lb for another 24 hrs
without any failure. This took the test to quitting time on Friday afternoon, so I just let the test
continue over the weekend to see what happened. I returned to a failure on Monday morning, so I don't know
exactly when it failed. But given that a 3/16" screw eye mounted in a properly sized pilot hole failed
immediately when a 40 lb weight was applied (photo 2), the difference in load carrying capacity was
dramatic in this application. This technique is well suited to side and back mounting applications.
I bonded two pieces of Sign-foam III™ HDU (the density of this foam is unknown, but Sign-foam III is
sold only in 10, 15 and 18 pcf) together to form a block of HDU 12" × 8" × 1½". I drilled a 15/16" hole
1¼" deep in the center of the block to receive a ½" cast eyebolt with 2 nuts. The outside points of the
nuts determined the size of the drilled hole. Using a 105/206/404 mixture, I mounted the hardware using
the procedure described above. I allowed this to cure for 24 hrs. I then built a support system and hung
weights from the eyebolt, beginning with 60 lb (photo 3) and loading the assembly in tension to represent
a top mounted sign. The sample didn't fail after 24 hrs, so I increased the load to 80 lb and after
another 24 hrs to 100 lb. After 72 hrs with the 100 lb load, the sample did not fail.
I then drilled a properly sized pilot hole and inserted a 3/8" threaded screw into the same block of HDU
and ran this set up through the same load scheme. I was quite surprised to learn that the foam held this
load and showed no signs of failure. This is quite a testament to the strength and integrity of the Sign-
foam III. I decided to press the issue and placed another 20 lb, bringing the total weight to 120 lb.
Still no failure. I was beginning to wonder if our technique was necessary. I remembered reading about a
sign maker who complained that his top mounted signs often failed in strong winds, so I decided to test
this by swinging the 120 lb of weight side to side. After about 3 back and forth cycles, the fastener
pulled free from the foam. Still, this isn't too shabby given the load of 120 lb. I doubt many foam signs
weigh that much. To be fair, I now reloaded the cast eyebolt and hung the same 120 lb from it and clamped
the rope to the eyebolt so the rope wouldn't simply rotate in the eye. This would force the side loads
into the bonded nut assembly. I spent about 10 minutes swinging this assembly pretty vigorously but
couldn't force a failure. I believe that this test showed the advantages of our bonding technique in a
"real world" application. And don't forget-the fastener can be removed and reinserted repeatedly without
any damage. The proper pilot hole sample performed quite admirably, but with repeated removals and the
cyclic loading from rocking in the wind, it would not perform to the level of a fastener that is bonded
in epoxy.
So what does all this mean?
From a practical standpoint, I would say that any sign maker knows that it gets expensive to keep
repairing signs that fail in their mountings. The cost savings realized in time and money for repairs
makes the WEST SYSTEM® fastener bonding technique a cost-effective alternative.
Epoxyworks 22 / Winter 2004
Copyright © 2003, Gougeon Brothers, Inc. All rights reserved.
This page is maintained by Gougeon Brothers, Inc. Last modified on (11/05/03).
Reproduction in any form, in whole or in part, is expressly forbidden without the consent of the publisher. EPOXYWORKS, Gougeon Brothers, WEST SYSTEM, Episize, Scarffer and Microlight as used throughout this publication, are trademarks of Gougeon Brothers, Inc., Bay City, Michigan, USA.
|