Common Errors in Fiberglass Laminate Repair

By Jeff Wright — Vice President of Technical Services

While most of our customers are successful when using WEST SYSTEM Epoxy to repair a damaged fiberglass laminate, we have become familiar with some common errors that are easily preventable. These mistakes are made by both professionals and amateurs. The information discussed in this article is available in our Fiberglass Boat Repair Manual and WEST SYSTEM User Manual, and on the WEST SYSTEM website.


Typical Fiberglass Laminate Repair

Object: Typical fiberglass repair cross-section. Action: Bevel ground at edge; fiberglass layers laid over epoxy; excess sanded away; final sanding. Context: hull repair, about 3 inches wide, 12:1 bevel. Transcribed text: Typical fiberglass repair Cross Section Excess glass sanded away Layers of fiberglass applied to equal the thickness A 12:1 bevel is ground on the edge of the repair and then final sanded with 80-grit paper Epoxy/fiberglass repair
A typical fiberglass laminate repair in cross-section.

This diagram illustrates how we recommend laminating a repair after the damaged fiberglass has been removed. It is critical that the scarf angle is at a minimum ratio of 12:1 and that the patch thickness matches the original laminate. Matching the original thickness ensures that the stiffness will be the same as the surrounding area, reducing the chance of a crack around the repair area.


Missing the root cause of the damage

A wall cross-section shows cracks radiating from impact points; exterior impact on the left, interior impact at center, with flex cracking around a bulkhead to the right. Exterior Impact Interior impact Flex cracking around bulkhead
Determine the root cause of the fiberglass laminate damage.

Finding the root cause of the damage can ensure that your repair holds up well for years. Stress cracks can help us understand what caused the damage. They may indicate whether something inside the boat has broken loose and caused the damage or if it was caused by something hitting the boat from the outside. The cracks can also point to a structural defect that must be corrected.


Not accounting for backside damage when estimating repairs.

Rock sample cross-section as the object. Action: shows impact damage; a diagonal black line overlays the specimen. Context: two labeled views: "Impact Side" (top) with concentric rings, and "Back Side" (bottom) with radiating fractures.
Check both the inside and outside of the core where damage has occurred.

With a cored composite, damage can be hard to evaluate when just looking at the outer skin. To fully assess the damage inner and outer skins and the core must be seen. These pictures show a fiberglass/wood/fiberglass laminate that looks only slightly damaged on the impact side, but the back side has a significant amount of broken fibers. When there is no access to the back side, you may need to grind away the outer skin and core to inspect the inner skin.


Poor adhesion caused by bonding to a damaged fiberglass laminate

Remove all damaged laminate before bonding.
Remove all damaged laminate before bonding.

Adhesion failure in the repair laminate is the most common failure mode for fiberglass repairs. To ensure good adhesion it is critical that the repair patch is adhered to undamaged laminate. This requires identifying and removing all damaged material.


Creating sharp corners when shaping the area to be repaired

A gray prohibition circle with a diagonal line overlays an irregular quadrilateral; to its right lies a separate elongated rounded-oval shape; both on a white background.
Shape the area to avoid sharp corners where stress concentrates

Corners can be described as stress concentrations. Machinists know this and avoid creating any sharp corners, machining a radius whenever possible. The same principle applies to fiberglass repair. Before grinding the scarf onto the surface, take the time to create a nice rounded shape to the repair area.


Inadequate scarf ratio Fig 6,7,8

Fig6

Fig8

scarf ratio
We suggest a minimum scarf ratio of 12:1 between the length of the scarf and the laminate thickness.

The scarf on the original laminate helps in many ways. It creates a substantial amount of surface area for adhesion and provides a transition zone so that the difference in properties of the new and original laminate are not concentrated at one point. We suggest a minimum 12:1 ratio between the length of the scarf and the laminate thickness. This ratio applies to both skins when repairing a cored laminate.


Damaging the surface of the repair area with excessive heat when grinding

Sketch of a hand grasping a computer mouse; the palm supports the device while the index and middle fingers rest on top, set on a flat desk.
Hand sand to avoid excessive heat from grinding, which can damage the laminate surface.

The removal of the damaged fiberglass laminate and creation of the scarf can be done with electric or pneumatic grinders and a 36-grit abrasive disc. Once everything is machined to the proper shape, the surfaces should be sanded by hand with 80-grit sandpaper. This is important because the high RPM power tools can generate significant heat that can soften the surface, resulting in a less-than-ideal surface profile for adhesion.


Contaminating the surface after it is sanded

A hand presses a small square pad onto a flat surface; to the left, a large circle with a diagonal line overlays a bottle, signaling no bottle use.
Take care not to contaminate a surface after sanding.

The final hand sanding with 80-grit sandpaper results in an ideal surface for WEST SYSTEM Epoxy adhesion. The sandpaper has exposed resin and fiberglass that has only been touched by the sandpaper so there are no contaminants on the surface. Wiping it with solvents increases the risk of introducing contamination either from the rag or a recycled solvent.


Vacuum bagging the repair laminate when unnecessary

The object is a negative-pressure wound-dressing kit. The dressing layers—foam sponge, breather fabric, release fabric, mastic sealant, vacuum bag film—are applied over a damaged area and connected to a vacuum canister via tubing. Text in image: - 12-to-1 bevel around damaged area - Vacuum bag film - Mastic sealant - Breather fabric - Release fabric - Fiberglass cloth - Mastic or adhesive - Plastic laminate - Vacuum gauge - Vacuum port
Don’t unnecessarily vacuum bag a fiberglass laminate repair.

When using a vacuum bag the surface that the bag is sealed against must be airtight. This can be difficult enough when using a mold so in the case of vacuum bagging to a laminate the risk of a leak is substantial. If there is a leak then too much epoxy will be pulled out of the laminate leaving a dry, weak repair patch. It is also important to match the thickness of the repair laminate to the original laminate. If the repair laminate is too thin from being compacted by a vacuum bag it may not be as stiff as the original laminate; if the repair is thicker than the original, it may be much stiffer which can concentrate stress around the perimeter, possibly resulting in cracks.


Failing to properly “map” the surface before applying fairing compound 

"Map" the fiberglass laminate surface before applying the fairing compound
“Map” the fiberglass laminate surface before applying the fairing compound

It is well worth spending the time to find the high and low spots before applying fairing compound. This is accomplished by using a long batten, as shown in the picture. When the high and low spots are defined it is easier to develop a strategy of what locations need fairing compound and where added thickness is not needed, resulting in less sanding. This also increases the likelihood that the repair will be fair with the unrepaired areas. The WEST SYSTEM Final Fairing & Finishing manual is an excellent guide to saving time and getting great results when finishing the repair.


Using only a palm sander to sand the surface, resulting in an unfair surface

An arc-shaped belt is clutched at both ends and pulled taut by two hands. In the background, radial shapes surround a vertical post, implying a demonstration or display setting.
“Map” the surface before applying the fairing compound

It is important to use a longboard when fairing large flat areas. In many cases, sanding tools designed for automotive bodywork will not work well because boats often have much larger areas to sand.  Also, in automotive work the original metal surfaces are much harder than the body filler. In fiberglass boat repair the repair area may have hardness very similar to the original laminate and you can accidentally change the shape of the surrounding area. Plan on using a variety of sanding tools if you are dealing with a repair that bridges both a flat area and a detailed area such as a chine or gunwale.


Discarding a reusable fiberglass laminate skin when replacing core

Rectangular lid is lifted off a shallow pan with a coarse interior and vertical-edge rim, set on a light surface.
Don’t discard a fiberglass laminate skin that could be reused.
A hand holds an electric hand sander, pressing its circular sanding pad onto a wooden work surface, smoothing the top of a bench.
Prepare the new core then bond the original fiberglass laminate skin back in place

A common fiberglass laminate repair is replacing a damaged core, often because of water absorption. In many of these repairs, the fiberglass “skins” are in great shape but need to be peeled off to replace the core. Bonding the original skin back onto the new core can save significant time and money. The only fiberglass required will be around the perimeter of the removed skin. This is a very nice technique when dealing with molded non-skid patterns.


Creating stress concentrations by not filleting corners and tapering laminates

The hand plane is being pushed along the edge of a wooden board, shaving thin wood to smooth the edge in a workshop.
Taper corners with filets
A hand holds a small rectangular card/scraper, pressing and smoothing a flexible sheet along a guide on a work surface, the sheet curving upward toward the edge.
Taper your fiberglass laminates.

Sharp corners can cause a problem in the laminate just like they can in the shape of the repair area. Smooth the transitions with thickened epoxy to make a fillet on inside corners. Also, when tabbing stringers and frames into place, taper the layers to create a nice thickness transition.


Applying an extra thick layer of fairing compound does not save time

A hand holds a rectangular card-like object against a rough rock surface.
Apply an extra thick layer of fairing compound doesn’t save time.

When fairing the repair, plan on applying at least three applications of fairing compound. Applying thick layers of fairing compound can trap air bubbles and cause you to lose the shape of the surface that you have carefully mapped as mentioned earlier. Although applying fairing compound in multiple layers may seem to take more time, you’ll actually spend less time sanding. Multiple layers will make it more obvious where the fairing compound needs to be applied.  We also recommend completing the fairing work with a thin coat of unthickened epoxy to provide a nice solid surface for the final finish.