Hog Tide Project

By Bruce Niederer — GBI Technical Advisor

The Hog Tide project began last summer when we partnered with Sail Magazine to produce a series of short videos showing how to repair an older J22 that I had arranged to be brought into the GBI Tech shop. The boat, named Hog Tide, needed the types of repairs we wanted to cover. The videos of the Hot Tide project can be found at both westsystem.com and sailmagazine.com.

If you’re wondering about the name, all the J22s that race in East Tawas, Michigan out of the Tawas Bay Yacht Club have ‘pig’ names—Pork Bellies, Pigs in Space, Pygmalion, Evil Dr. Porkchop, The Other White Meat, and my favorite, Notorious P.I.G., are notables.

This article features still pictures taken while the videos were being shot. I’ll comment as we walk through the process.

The bulkhead we were replacing had a lot of checked and rotten areas around each chainplate. There was rot just about everywhere except for the trim piece, which we removed and saved to re-install on the new bulkhead.

The forward interior of a small boat shows a central metal pole spanning a V-shaped hull, with worn white fiberglass, wooden trim, and a red deck label (text unreadable).

To remove the bulkhead intact, I used a vibrating side cutter with a diamond grit blade. This allowed the bulkhead to be removed full size so we could trace the shape for the new bulkhead.

The back-side tabbing was left in place to make the alignment process a no-brainer when we installed the new bulkhead.

Interior of a small fiberglass boat with the hull exposed; a metal post stands near a coiled hose and a portable tool on a wooden deck, sunlight entering through openings. A large plywood panel stands upright on a workshop floor, featuring a white, semi-circular arch inset with brown rust-stained edges. The area shows worktables, tools, and taped floor lines indicating fabrication.

Had the bulkhead not come out so cleanly, we would have needed to make a template from scratch for the bulkhead. Tom demonstrates how to make an accurate template by fitting some cardboard loosely then stapling small wooden strips extending to meet the hull of the boat to define the exact shape needed. Tom laid out the template and made tick marks at the end of the wooden sticks on the sheet of marine-grade plywood. Then, using a flexible batten, it was simply a game of connect the dots to define the shape of the bulkhead.

Curved brown cardboard panel is being positioned and stitched along its edge by an older man inside a boat hull, with the deck and a metal support frame around him. Curved brown corrugated cardboard is clamped along its edge by white plastic strips with small metal pins, laid across a light plywood work surface. Object: a hand holding a pencil; Action: marking a line along a thin wooden strip on light plywood; Context: a workshop with several strips pinned across the surface.

Once our new bulkhead was cut out, it was ready for 6 oz. fiberglass to be laminated to both sides. After curing overnight, all surfaces that would receive epoxy were prepped using an abrasive pad so as to not damage the fibers of the fiberglass, but still scuff up between the weave of the fabric.

To install the new bulkhead, I precut enough 727-4 Biaxial 4″ tape for the tabbing then shanghaied Tom to be my “ground crew” while I worked inside the boat.

Curved pale foam panels rest on a white workshop table; scissors lie nearby, with tools and a red machine visible in the background.

Tom supplied me with 105 Resin/206 Slow Hardener filled to a non-sag consistency with 403 Microfiber filler. We chose to use the 403 because it thickens fast without much airborne dust while mixing. The resulting graininess of the fillet would be glassed over anyway, so cosmetics were not an issue.

We applied thickened epoxy to the flange (original tabbing) we’d left intact, then clamped the bulkhead to the flange drawing it into perfect position. This allowed me to apply a fillet to the perimeter of the part—with the exception of the limber hole along the centerline—water still needs to flow into the bilge from the bow area.

Orange clamps grip a vertical metal rod across a curved plywood form inside a workshop; a cordless drill rests nearby, with a round hole and dusty gray interior surrounding.

Once the fillets got a bit tacky, the 727 glass tape tabbing was installed—again using 105/206. Note that we used several shorter lengths of glass tape to make the curve and overlapped them a bit. This kept the glass from buckling around the curve and eliminated the need to cut pleats in the glass.

A curved wooden bulkhead is bolted along the interior of a boat hull; a metal support post stands nearby, with a green rag on plywood inside the unfinished cockpit. Central metal post rises from wooden deck, with a ring at the top; inside a boat cabin with curved white walls, wooden floor panels, and a coiled rope to right.

Shortly after we’d completed the transom replacement (along with some other repairs) Hog Tide was returned to her owner and took first place out of eight J/22s racing on Lake Huron’s Tawas Bay just a few weeks later.